Process Mechanism Of TOPCON Solar Panels in Various Processes Part 3

Dec 16, 2024 Leave a message

640

 

 

 

Annealing

 

 

Place the silicon wafer in a reaction tube made of quartz glass, which is heated to a certain temperature using a resistance wire heating furnace (the commonly used temperature is 900-1200 ℃, which can be reduced to below 600 ℃ under special conditions). When oxygen passes through the reaction tube, a chemical reaction occurs on the surface of the silicon wafer:

 

Si (solid)+O2 (gaseous) → SiO2 (solid)

 

The redistribution of impurities generated during the annealing process also plays a role in impurity absorption, utilizing PSG's adsorption and fixation of sodium and potassium ions to remove these harmful ions.

 

Analysis of pollution generation links: The main pollution links in this process are residual oxygen and nitrogen in the thermal oxygen link.

 

 

 

 

BOE cleaning

 

 

The BOE (5-line) slot type equipment is an integrated semi closed device, where silicon wafers are placed in baskets by automated equipment and converted into solutions in each slot of the equipment through mechanical arms. The chemical tank is continuously replenished with corresponding chemicals based on the concentration of the solution and regularly replaced as a whole. The replaced waste liquid is discharged into the wastewater system and ultimately enters the sewage treatment plant for treatment. The washing tank is cleaned with purified water. When there are silicon wafers in the tank, purified water is slowly added, and the salt containing wastewater automatically overflows to the wastewater collection system and finally enters the sewage treatment plant for treatment. All chemicals are in liquid form and are automatically dispensed by a diaphragm pump. The cleaning sequence is: pickling tank * 2, water washing, post pickling (HCl/HF/DI), water washing, slow pulling, drying * 6, with a tank size of 720L.

 

 

1) Acid washing

 

A dilute acid solution (3.15% HCl and 7.1% HF) is required for high-purity cleaning. The function of HCl is to use Cl - to complex metal ions, while the function of HF is to remove the oxide layer on the surface of the silicon wafer, making it more hydrophobic and forming the silicon complex H2SiF6. By coordinating with the metal ions, the metal ions are detached from the surface of the silicon wafer, reducing the metal ion content of the silicon wafer. HF acid washing is carried out for 150 seconds to remove the BSG layer on the front and PSG layer on the back. After acid washing, pure water cleaning is performed.

 

HF+SiO2→SiF4+H2O

 

SiF4+HF→H2SiF6

 

 

2) Post pickling

 

After post cleaning, a dilute acid solution (14.7% HF) should be used for high-purity cleaning. The function of HF is to remove the oxide layer on the surface of the silicon wafer, making it more hydrophobic and forming the silicon complex H2SiF6. Through the complexation with metal ions, the metal ions are detached from the surface of the silicon wafer, reducing the metal ion content of the silicon wafer.

 

The chemical reactions that occur during the pickling process are as follows: SiO2+6HF=H2SiF6+2H2O

 

The working temperature of the pickling tank is at room temperature, and the pickling time is controlled at 100 seconds.

 

 

3) Drying

 

Transfer the slowly pulled pre dehydrated crystalline silicon wafer to a drying tank, and blow hot air at 90 ℃ up and down on the wafer for drying, using electric heating.

 

The above acid washing process will produce high concentration acidic wastewater containing HCl and hydrofluoric acid (W21) and high concentration acidic wastewater containing hydrofluoric acid (W23), and generally acidic cleaning wastewater (W22, 24, 25). The above operation is carried out in a closed cleaning machine, and the acid washing process will volatilize to produce acidic waste gas containing HCl and HF (G6) and acidic waste gas containing HF (G7), which will be collected through pipelines and sent to the acidic waste gas washing tower for treatment.

 

 

 

 

ALD

 

 

Use ALD equipment to deposit a layer of Al2O3 on the surface of silicon wafers to improve their passivation and impurity absorption effects. The main method is to react gaseous Al (CH3) 3 with water vapor (H2O) to generate Al (OH) 3, which adheres to the surface of silicon wafers and produces methane gas.

 

The main reaction equation is:

 

Al(CH3)3+3H2O→Al(OH)3+3CH4↑

 

2Al(OH)3→Al2O3+3H2O↑

 

The ALD equipment is a closed negative pressure device, equipped with an inlet, outlet, and inlet/outlet. The heating is electric heating, and the equipment comes with an oil-free dry mechanical vacuum pump. After production begins, the robotic arm first sends the battery cells into the ALD equipment and closes the feeding port. Heat to a certain temperature, evacuate, and bring the pressure inside the equipment to the required level for production. By alternately introducing the gas-phase precursor TMA and H2O pulses into the reaction chamber, and chemically adsorbing and reacting on the deposition substrate, a deposition film AL2O3 is generated. Finally, the methane exhaust gas inside the equipment is replaced with nitrogen gas, and the equipment is turned on to automatically remove the silicon wafer.

The main pollutant in this process is exhaust gas methane (G8), which is extracted by a vacuum pump and treated by a stainless steel silane combustion cylinder and water spray device.

 

 

 

 

Front coating

 

 

The basic principle is to use high-frequency light discharge to generate plasma that affects the thin film deposition process, promotes the decomposition, combination, excitation, and ionization of gas molecules, and promotes the generation of reactive groups. Due to the presence of NH3, it facilitates the flow and diffusion of active groups, increases the growth rate of thin films, and greatly reduces the deposition temperature.

 

The main chemical reactions that occur during the PECVD deposition of silicon nitride oxide films are:

 

SiH4+NH3+N2O→xSi2O2N4+N2↑+yH2↑

 

The PECVD positive film equipment is a closed negative pressure device, electrically heated, and comes with an oil-free dry mechanical vacuum pump. During production, nitrogen is first filled into the equipment, and the robotic arm completes the silicon wafer loading. After the equipment reaches external pressure, the inlet and outlet are opened, and the graphite boat automatically enters the equipment and closes the inlet and outlet. Vacuumize and conduct various safety checks. After confirming safety, introduce silane and ammonia gas to complete the nitrogen oxide silicon coating inside the equipment. After the coating is completed, the residual gas in the special gas pipeline and equipment is discharged through nitrogen gas, and then the inlet and outlet are opened for discharge. After cooling, enter the sorting process and proceed to the subsequent process.

 

Analysis of Pollution Production Process: The main form of pollution in this production process is coating waste gas (silane, excess laughing gas, excess ammonia, hydrogen, nitrogen, etc.) (G9), which is first treated in the stainless steel silane combustion cylinder through the induced draft system, and then discharged after being treated by the spray tower.

 

6401

 

 

 

 

Back coating

 

 

The main chemical reactions that occur during the PECVD deposition of silicon nitride oxide films are:

 

SiH4+NH3+N2O→xSi2O2N4+N2↑+yH2↑

 

The PECVD back film equipment is a closed negative pressure device, electrically heated, and comes with an oil-free dry mechanical vacuum pump. During production, nitrogen is first filled into the equipment, and the robotic arm completes the silicon wafer loading. After the equipment reaches external pressure, the inlet and outlet are opened, and the graphite boat automatically enters the equipment and closes the inlet and outlet. Vacuumize and conduct various safety checks. After confirming safety, introduce silane and ammonia gas to complete the nitrogen oxide silicon coating inside the equipment. After the coating is completed, the residual gas in the special gas pipeline and equipment is discharged through nitrogen gas, and then the inlet and outlet are opened for discharge. After cooling, enter the sorting process and proceed to the subsequent process.

 

Analysis of Pollution Production Process: The main form of pollution in this production process is coating waste gas (silane, excess laughing gas, excess ammonia, hydrogen, nitrogen, etc.) (G9), which is first treated in the stainless steel silane combustion cylinder through the induced draft system, and then discharged after being treated by the spray tower.

 

 

 

 

Metalization

 

 

1) Printing

 

During the printing process, the slurry is above the screen, and the scraper is pressed onto the screen with a certain pressure, causing the screen to deform and come into contact with the surface of the silicon wafer. The slurry is extruded and comes into contact with the surface of the silicon wafer; The surface of the silicon wafer has a strong adsorption force, which forces the slurry out of the mesh holes. At this point, the scraper is running, and the previously deformed mesh plate, under good restoring force, allows the slurry to smoothly fall onto the surface of the silicon wafer. Silver paste is a paste like printing paste made from ultra-fine and high-purity silver and aluminum powder as the main metal, supplemented with a certain amount of organic binder and resin as auxiliary agents.

 

Firstly, back electrode printing and drying: Accurately locate and print the back electrode paste (including laser drilling positions) (silver paste) on the back of the battery, and quickly dry it at low temperature to ensure that the printed back electrode is not damaged during the next printing step.

 

Secondly, printing and drying of fine grid lines on the back: Accurately position and print fine grid line paste (silver paste) on the back of the battery, and quickly dry it at low temperature. The main purpose is to contact the silicon substrate, transmit current, and re dope to reduce carrier recombination and increase boost.

 

Then, after passing through the flipper, the battery cells are flipped from the back to the front facing upwards. Perform positive electrode printing and drying: Accurately position and print positive electrode paste (silver paste) on the front of the battery, and quickly dry it at low temperature. Its main function is to conduct and transport the current collected by the fine grid lines to external circuits or memory.

 

Finally, printing and drying of the front fine grid lines: Accurately position and print the paste (silver paste) of the front electrode on the front of the battery. After printing, wait for it to enter the sintering furnace for solid sintering, forming a good ohmic contact. Its main function is to collect current, increase the light absorption capacity of the battery cell, and improve conversion efficiency.

 

The drying temperature of the slurry during the above drying process is around 200 ℃. This process will generate organic volatile gases (G10), with the main pollutants being alcohol esters such as dodecane, calculated as VOCs. The organic waste gas generated during the printing process is collected by a gas collection hood and treated by a two-stage series connected activated carbon adsorption box, and finally discharged through an exhaust pipe. The exhaust duct needs to be regularly cleaned and cleared to maintain its absorption efficiency.

 

 

2) Sintering

 

Sintering is the process of sintering the main fine gate paste printed on a silicon wafer into a battery cell at high temperatures, allowing the electrode to be embedded on the surface, forming a strong mechanical contact and good electrical connection, ultimately resulting in an ohmic contact between the electrode and the silicon wafer itself.

 

Printed silicon wafers are sintered using an electric heating furnace, which is divided into different temperature zones. During the sintering process, the silicon wafers form upper and lower electrodes, and the highest sintering temperature is between 700~800 ℃. During this process, the organic solvents such as alcohol ester dodecane in the slurry completely evaporate to form organic waste gas (G11), which is calculated as VOCs. Then, it is fully burned and treated by the equipment's built-in high-temperature combustion tower device, and together with the printing waste gas, it is adsorbed and treated by a two-stage series connected activated carbon adsorption box. After adsorption, it is discharged through the exhaust pipe.

 

 

3) Electric injection

 

After sintering the battery cells, the method of directly injecting charge carriers (reverse injection of direct current) is used to change the charged state of hydrogen in the silicon body, which can effectively passivate the decaying boron oxygen complex and transform it into a stable regenerated state, ultimately achieving the goal of anti light decay.

 

 

 

 

Test packaging

 

 

After the completion of solar cell production, testing instruments will be used to test the electrical performance parameters of the solar cell (such as measuring its I-V curve and light conversion rate). After the test is completed, the battery will be automatically divided into multiple levels according to certain standards. When the number of battery cells in a certain level reaches the specified limit, the device will remind the operator to take them out for packaging. The device also has a fragment detection function, which promptly removes fragments upon discovery, rather than testing them as complete batteries, resulting in waste battery cells (S2).